Example 3
Moulded Silicone Pressure Sensitive Adhesive Body:
Dow Corning 7-9800 A&B (mixing ration between A and Bis 1:1 by weight) were used for production of a PDMS based adhesive body. A mould having a triangular shape (each side of the triangular mould having a distance of 300 mm, the center part having a thickness of 0.5 mm and the edge having a thickness of 0.1 mm) was used. The components were thoroughly mixed and applied on a 50 μm cover layer of silicone rubber lining in the female part of a triangular mould and a male mould part was placed on top, said part lined with a low density polyethylene release liner. The adhesive was cured in an oven at 100 degree C. for 15 minutes. After curing the adhesive was punched out of the mould and a dent in the centre of the adhesive body device for embedment of an electronic sensing system was punched out.