Example 5

HA was transferred to plastic jars. A 2.5% (w/w) NaOH solution was mixed with BODE in a shaker with an HA concentration of 18% (w/w) of the final mixture. The jars were transferred to an incubator or a water bath to perform the cross-linking step for 24 h, 48 h or 72 h, respectively, at RT.

The resulting gels were allowed to swell to 20 mg/g HA in a buffer solution containing sodium phosphate, HCl and NaCl, at a pH about 7.5. The gels were filled in syringes and then autoclaved.

Results:

Cross-linking time (h)G′ (Pa)
2475
4819
721

The cross-linking reaction yields a gel with particularly useful properties, e.g. gel strength, for reaction times of less than 48 h, such as 24 h.